Synthesis of Chitosan-PEI
Jump to navigation
Jump to search
Copolymer of CP was prepared according to the methods described by Gao et al. [8].
Dissolve 0.5 g Chitosan in 20 ml of a 0.5% acetic acid solution
Adjust to pH 7.0
Stir overnight.
Add CDI 1,19-carbonyldiimidazole (pierce) at a molar ratio of CDI:CS amine = 2:1
http://www.sigmaaldrich.com/catalog/product/aldrich/21860
21860-5G, 29.00, 21860-25G 83.10
Stir for 1 h.
Add PEI (1.8 kDa) dropwise into the solution under stirring at a molar ratio of PEI:amine = 2:1.
Polymerize at room temperature (25uC) overnight.
Dialysis in water for 48 h.
Collect the powder by lyophilization.